AKD (Alkyl Ketene Dimer) delivers superior acid resistance and simple bulk storage for liquid packaging and slower machines, while ASA (Alkenyl Succinic Anhydride) cures instantly on-machine for high-speed paper production. Choosing between them comes down to your machine speed, size press setup, and mill white-water hardness.
When North American paper mills shifted away from acid rosin-alum sizing to alkaline papermaking, AKD and ASA became the industry standard. Both chemicals allow mills to run high-brightness precipitated calcium carbonate (PCC) fillers at neutral-to-alkaline pH levels.
Picking the wrong sizing agent for your specific machine costs more than chemical dollars. A poor match leads to sticky press-section deposits, blown size press sheets, or slippery reels that jam high-speed office printers.
AKD vs. ASA Sizing: Quick Technical Comparison
Before diving into reaction mechanics, here is how both reactive sizing agents stack up on a standard paper machine floor.
| Performance Factor | AKD (Alkyl Ketene Dimer) | ASA (Alkenyl Succinic Anhydride) |
| Chemical Delivery | Pre-emulsified liquid (10%–20% solids) | 100% active amber oil |
| Emulsification | Ready to dose from bulk tank | Must be emulsified on-site |
| Curing Speed | Slow (40%–60% at reel; 24–72 hrs full cure) | Ultra-fast (85%–95% cured on-machine) |
| Hydrolysis Byproduct | Waxy, inert dialkyl ketone | Sticky calcium/magnesium salts |
| Ideal Operating pH | 7.5 to 8.5 | 6.8 to 8.0 |
| Max Storage Temp | Below 86°F | Emulsion kept below 85°F–95°F |
| Typical Active Dosage | 1.5 to 4.0 lbs per short ton | 1.5 to 3.0 lbs per short ton |
| Best Paper Grades | Liquid packaging board, fine paper | Copy paper, linerboard, gypsum liner |
The Wet-End Chemistry: How AKD and ASA Bond to Cellulose
Cellulose fibers naturally love water because their surfaces are packed with polar hydroxyl (-OH) groups. Internal sizing works by chemically anchoring a water-repellent fatty hydrocarbon tail directly onto those hydroxyl groups, turning a sponge-like web into a controlled barrier.
Both AKD and ASA are cellulose-reactive molecules, meaning they form actual covalent bonds with the fiber. The difference lies in the shape of their reactive rings—and what happens when they react with water instead of wood fiber.
How AKD Reacts in the Sheet
AKD is built around a four-membered lactone ring attached to two long fatty acid chains (typically C16 to C18). Inside the dryer section, heat causes this ring to open and bond with a cellulose hydroxyl group, creating a stable beta-keto ester.
Because AKD’s lactone ring is relatively stable, it reacts slowly. If an AKD molecule reacts with water instead of cellulose (hydrolysis), it forms an unstable acid that sheds carbon dioxide and turns into a dialkyl ketone.
That ketone does not size the paper, and too much of it makes the sheet waxy and slippery. However, it is chemically inert and rarely creates the gummy pitch deposits that shut down press sections.
How ASA Reacts in the Sheet
ASA features a five-membered succinic anhydride ring bonded to an unsaturated carbon chain. That five-membered ring carries high molecular strain, making it aggressively reactive toward cellulose hydroxyl groups.
As soon as the sheet hits the dryer cans, ASA forms a covalent ester bond almost instantaneously. The downside of this high reactivity is that ASA attacks water just as aggressively as it attacks fiber.
When ASA hydrolyzes in the headbox or white-water loop, it forms alkenyl succinic acid—a dicarboxylic acid. In hard mill water, that acid binds with free calcium and magnesium ions to form insoluble, tacky calcium salts that stick tightly to forming fabrics, press felts, and Uhle boxes.
Curing Speed and Size Press Runnability
If your mill runs a high-speed uncoated freesheet machine with an on-machine metering size press, curing speed dictates your entire day. ASA consistently achieves 85% to 95% of its full sizing value before the sheet ever reaches the size press.
That instant cure keeps the sheet strong enough to absorb surface starch without losing wet strength and snapping in the draws. It also gives lab technicians reliable, immediate feedback when running TAPPI T 441 (Cobb Sizing Test) or TAPPI T 530 (Hercules Sizing Test / HST) right off the reel.
Absorption Tester
Cobb Sizing Water Absorption Tester for Paper, Cardboard & Corrugated Packaging
Measure surface water absorption (Cobb values) quickly to verify AKD curing progress and ASA reel-end sizing consistency across fine paper, paperboard, and corrugated packaging grades.
- Tests paper, cardboard & paperboard
- Built for corrugated packaging QC
- Verifies AKD & ASA sizing performance
- Essential for mill & converting labs
AKD behaves differently. Even with dryer cylinder temperatures running between 195°F and 230°F, an AKD-sized sheet typically leaves the reel at only 40% to 60% of its ultimate sizing potential.
Full AKD cure often takes 24 to 72 hours inside the wound roll, unless you dose cationic polyamine cure promoters. Mills running AKD often have to run an oven-curing step in the quality lab just to predict next week’s final Cobb values.
Water Hardness, Closed Loops, and Deposit Control
Water chemistry makes or breaks an ASA program, especially as mills tighten their water loops to meet U.S. EPA Effluent Guidelines and sustainability targets. Older open-loop mills used 10,000 to 15,000 gallons of fresh water per ton of paper, whereas modern closed-loop recycled containerboard mills often operate below 2,500 gallons per ton.
Tightening that loop concentrates dissolved calcium, magnesium, and sulfate ions in the white water. According to U.S. Geological Survey (USGS) water hardness standards, water is classified into four distinct brackets:
- Soft: 0 to 3.5 GPG [0 to 60 ppm (mg/L)]
- Moderately Hard: 3.5 to 7.0 GPG [61 to 120 ppm (mg/L)]
- Hard: 7.0 to 10.5 GPG [121 to 180 ppm (mg/L)]
- Very Hard: Over 10.5 GPG [over 180 ppm (mg/L)]
When white-water hardness climbs above the USGS “Very Hard” threshold of 10.5 GPG [180 ppm (mg/L)]—and recycled mills routinely see 15 to 25 GPG [257 to 428 ppm (mg/L)]—unretained ASA becomes a serious liability. Any hydrolyzed ASA floating in the white water instantly precipitates as sticky calcium salts.
To survive high-hardness loops with ASA, wet-end chemists maintain first-pass retention above 80% and dose small amounts of liquid aluminum sulfate (alum) or polyaluminum chloride (PAC) to fix hydrolyzed ASA onto fibers before it reaches the felts. AKD, by contrast, shrugs off hard water far more easily, making it a safer bet for heavily closed recycled board mills with high dissolved solids.
Total Water Hardness Titration Kit (GPG & mg/L)
Spot calcium buildup before it crosses the 10.5 GPG [180 ppm] threshold and turns hydrolyzed ASA into sticky felt deposits.
- Reads directly in GPG and ppm (mg/L)
- High-range titration for closed recycled loops
- Fast benchtop or machine-floor testing
Industrial Non-Contact Infrared Thermometer (°F/°C)
Monitor ASA emulsion lines (keep under 85°F–95°F), AKD bulk tanks (below 86°F), and dryer cylinder surfaces in seconds.
- Instant °F readings for piping & tanks
- Dual-laser targeting for safe distance checks
- Rugged housing for humid wet-end floors
Equipment, Storage, and Total Mill Cost
When plant managers compare chemical invoices, ASA looks cheaper per pound of active ingredient because dosage rates sit around 1.5 to 3.0 lbs per short ton. However, active chemical price only tells half the economic story.
ASA arrives as a 100% active oil and cannot be pumped straight into the stock approach system. Your mill must buy or lease a high-shear turbine emulsification skid, maintain a cationic starch cooking system (often holding 1,000 to 3,000 gallons of cooked starch), and engineer tight piping so the fresh emulsion enters the fan pump in under 15 to 20 minutes.
Temperature control is equally strict. If the emulsion water rises above 95°F, ASA hydrolyzes before it even touches the pulp, wasting chemical and triggering felt-plugging deposits.
AKD requires almost zero capital overhead. Suppliers deliver it as a milky-white, pre-emulsified dispersion straight into a standard 3,000- to 6,000-gallon fiberglass bulk tank.
You simply meter it out with a standard positive-displacement pump at roughly 1.5 to 3.0 gallons per short ton, depending on emulsion solids. As long as your bulk tank stays below 86°F and turns over within 30 to 90 days, AKD remains remarkably low maintenance.
Choosing by Paper Grade: Where Each Agent Wins
Neither chemical is universally better; each dominates specific sectors of the North American pulp and paper market.
When to Choose AKD Sizing
- Liquid Packaging Board (LPB): Milk cartons and aseptic juice boxes require extreme resistance to edge-wicking from lactic acid and hot hydrogen peroxide sterilizers. AKD’s beta-keto ester bond holds up against acidic liquids far better than ASA.
- Low-Capital or Slower Machines: Specialty mills running under 2,500 feet per minute rarely justify the maintenance and equipment footprint of an on-site ASA emulsification unit.
- High-Hardness Recycled Furnish: Mills battling white-water hardness over 15 GPG [257 ppm (mg/L)] with fluctuating anionic trash enjoy cleaner press felts and fewer wash-ups with AKD.
When to Choose ASA Sizing
- High-Speed Uncoated Freesheet: Copy paper and offset printing machines running 4,000 to 5,500 feet per minute need ASA’s instant cure for stable size press runnability.
- Strict Coefficient of Friction (COF) Specs: Overdosing AKD creates waxy ketones that cause high-speed laser printers to double-feed sheets. ASA leaves a higher surface friction and promotes cleaner toner adhesion.
- Gypsum Board Liner and Containerboard: Fast-converting packaging grades benefit from ASA’s lower dosage rates, predictable reel-end Cobb testing, and quick grade transitions.
Conclusion: Matching Sizing Chemistry to Your Paper Machine
If your operation demands rapid on-machine curing, crisp toner adhesion, and zero sheet slippage at high speeds—and you have the retention program and starch infrastructure to support on-site emulsification—ASA delivers the best performance per ton. If you produce liquid packaging, run heavily closed recycled water loops above 10.5 GPG [180 ppm (mg/L)], or want plug-and-play bulk storage without deposit headaches, AKD remains the smarter workhorse.
Before committing to a wet-end trial, audit your white-water hardness, check your dryer temperature profile, and measure your true first-pass retention. Matching the chemistry to your machine’s physical reality always beats chasing the lowest price per gallon.
Frequently Asked Questions (FAQ)
Can a paper mill switch from AKD to ASA without major downtime?
Switching from AKD to ASA requires installing an on-site high-shear emulsification unit, a stabilizer feed line (cationic starch or synthetic polymer), and chilled dilution water lines. While the wet-end stock changeover takes only a few hours during a planned boil-out, installing the mechanical skid usually requires a scheduled maintenance outage.
Why does AKD sizing sometimes cause slippery paper on the winder?
When AKD is overdosed or fails to react with cellulose fibers, excess molecules hydrolyze into waxy dialkyl ketones. These ketones migrate to the sheet surface during drying, lowering the paper’s coefficient of friction and causing telescoping rolls on the winder or double-feeding in office copiers.
What temperature ruins an ASA emulsion in the mill?
ASA emulsions should be kept below 85°F to 95°F and used within 15 to 20 minutes of emulsification. Higher temperatures drastically accelerate hydrolysis, turning active ASA into non-sizing dicarboxylic acid that causes sticky press-section deposits.
Which sizing agent performs better in high-PCC (calcium carbonate) sheets?
Both AKD and ASA work well with precipitated calcium carbonate (PCC), but ASA offers tighter sizing control during rapid grade changes. However, high PCC levels increase free calcium ions in the white water, so ASA systems must pair with strong retention aids to prevent calcium salt buildup.